Molecular SieveZeolite AdsorbentsBy SorbiTech™
Twin adsorber towers of a gas treating unit

Molecular Sieve Regeneration Temperature, Hold and Cooling

Purge temperature by grade and duty, and how the heating, hold and cooling steps are run.

Related Solutions

Quick Answer

Molecular sieve regeneration temperature is the temperature of the dry purge gas that drives adsorbed water off the bed, typically 200 to 315 °C (390 to 600 °F) at the vessel inlet depending on grade and duty. The hot step is followed by a hold until the bed outlet nears the inlet value, and then by cooling with the heater bypassed.

  • Grades 3A, 4A, 5A and 13X
  • Water capacity by gravimetric uptake
  • Manufactured by Medaad

Request the TDS Request the SDS

Engineering GuideUpdated

Beds that dry reactive olefin streams run at the cool end of that band, while natural gas dryers commonly regenerate near the top of it. Most designs keep the inlet below about 325 °C, because higher heat starts to damage the crystal. The sections below explain why each value is chosen, how the cycle is run and what goes wrong when it drifts.

How Heat and Dry Purge Gas Release Water

A zeolite crystal holds water inside cavities joined by pores of a fixed width, a structure described in how a molecular sieve sorts molecules. At ambient temperature the pull on each water molecule is strong, which is why the sieve can dry gas to below 1 ppmv. That pull weakens as the temperature rises. At regeneration temperature the bed can hold only a small part of what it held cold, so the surplus water leaves the crystal as vapour.

Heat alone is not enough. The released vapour has to be carried away, or the sieve would take it up again as it cools. A dry purge gas does both jobs. It brings heat into the bed and sweeps the water out of the vessel. The drier the purge, the less water stays on the sieve at the end of heating, and the drier the product gas in the next adsorption step. That leftover load sets the dew point a bed can reach, which is why it is fixed early in molecular sieve bed design for dryers.

Regeneration Temperature by Grade and Duty

The temperature depends on what the bed holds and how strongly it holds it. Water in the small pore of 3A molecular sieve leaves at a moderate heat, which suits feeds that react on hot beads. Sieves that also hold sulfur compounds or carbon dioxide need more heat. The values below are purge temperatures at the vessel inlet. They are typical values, for guidance only.

DutyUsual gradeTypical purge inlet temperatureWhat sets the value
Cracked gas and olefin drying3A200 to 230 °CA cooler purge limits reaction of olefin traces on hot beads
Natural gas dehydration4A or 3AAbout 280 to 315 °CThe outlet dew point required and the heat available on the plant
Mercaptan removal13XHold at 180 to 200 °C for one to two hours, then about 280 °CMercaptans are swept out before the bed reaches the heat that breaks them down
First activation after loadingAll gradesAbove 250 °C, about 230 °C for 3AWater picked up from the air while the vessel stood open

Olefin units, covered under petrochemical olefin purification, keep to the low row because hot beads can start polymerising traces in the feed. Where the feed carries H₂S, as in sour gas dehydration, the temperature is a balance between stripping the sulfur and limiting side reactions. Choosing the grade in the first place is set out in 3A vs 4A molecular sieve and where 5A and 13X fit.

Heating, Hold and Cooling Steps

A thermal swing cycle has three steps. Heating raises the bed to the target temperature, a hold keeps it there until the whole bed has given up its water, and cooling follows with the heater bypassed. Figure 1 traces the purge inlet and the bed outlet temperature through one cycle.

Figure 01 · Purge inlet and bed outlet temperature through heat, hold and cool
TEMPERATUREPURGE INLETWATER PLATEAUBED OUTLETOUTLET NEARS INLETHEATHOLDCOOLSWITCHTIME

The outlet trails the inlet. It pauses while most of the water leaves, then climbs. Heating ends once the outlet is close to the inlet value. The bed is switched only after the outlet has cooled.

The inlet temperature is raised gradually over one to two hours. The outlet trails behind. It climbs quickly at first, then flattens into a plateau while most of the water evaporates, then climbs again toward the inlet value. The plateau shows the drying front moving through the bed. Heating usually ends once the outlet is within about 20 °C of the inlet and has stayed there for the set hold time. A heating period of about five hours is common on gas dryers.

The outlet should always read below the inlet, because the vessel and piping lose heat. An outlet that suddenly climbs faster than expected points to a heat releasing reaction inside the bed, and heating is stopped at once. Cooling then runs until the outlet is close to the operating temperature, often within about 15 °C. A bed switched while still hot releases a brief spike of water or impurity, and on a reactive feed it can start a reaction. The sieve is a good insulator, so a bed left part cooled after a shutdown can stay hot for weeks.

Purge Gas Flow Direction and Source

Adsorption usually runs downward through the bed. The heating gas enters at the bottom and flows upward, counter current to adsorption. This sends heat first into the dry product end, the end that must be cleanest when the bed returns to service. Water pushed ahead of the heat leaves through the top, the end that was already wet. Cooling with dry gas normally runs the same upward way, so the bottom of the bed never meets moisture. Where wet feed gas is used for cooling, the flow is reversed so any water it leaves sits at the inlet end.

The purge is most often a slipstream of dry product gas, taken after the dryers, heated, passed through the bed, then cooled to condense the water. In many oil and gas processing plants the spent regeneration gas is recompressed and returned to the inlet, or sent to fuel. The purge flow must be high enough to spread evenly across the bed, since a weak flow channels and leaves wet pockets. Air plants follow the same logic, using dry waste nitrogen from the cold box as purge in air prepurification.

Capacity Loss From Too Cool or Too Hot a Purge

A purge that is too cool, too short or too wet leaves water on the sieve. The bed then starts each adsorption step partly loaded, so breakthrough comes earlier and the outlet dew point drifts up. Ahead of a cryogenic section, as in LNG pretreatment, that drift can freeze exchangers.

Heat that is too high, or a ramp that is too fast, causes different damage.

  • Steaming. Water driven quickly off the lower bed condenses again in the cooler upper bed, then boils off once more. That hot liquid water attacks the crystal and the binder. It is the main cause of hydrothermal ageing, described in what shortens molecular sieve lifetime.
  • Coking. Heavy hydrocarbons and olefins left on the beads crack into carbon at high temperature and block the pores.
  • COS formation. In sour gas, H₂S and CO₂ on hot sieve can react to form carbonyl sulfide (COS) and water. More H₂S and CO₂ and a hotter regeneration both increase it. The COS tends to end up in the propane product, which then needs treating, as covered in LPG and NGL treating. 3A grades with low reactivity are often chosen to limit the reaction.

Tower Count, Cycle Length and Heater Duty

The simplest molecular sieve dehydration unit has two towers, one drying while the other is heated and cooled. Larger gas plants often use three or more, with two in adsorption and one in regeneration. Adsorption steps of about eight hours or more are common, and heating, cooling and any standby must all fit inside that time. Shorter steps need less sieve and smaller vessels, but they mean more heating cycles per year, more valve operations and usually a shorter charge life.

The heater is sized in outline from three loads. It heats the sieve, heats the steel of the vessel and its internals, and supplies the heat that releases the water. On large vessels the steel shell also takes up a large share of the heat, which is one reason internal insulation is sometimes fitted, a choice made in adsorber vessel design. The purge flow is then chosen so the bed reaches temperature within the heating time. The regeneration cooler and separator are sized to condense and remove the water that leaves. How these pieces fit together is shown in molecular sieve dehydration systems.

Pressure Swing Regeneration Without a Heater

A pressure swing adsorption (PSA) unit clears its bed by dropping the pressure and purging with a little product gas. No heater is used, and a full cycle takes minutes. The method suits gases held lightly, which leave as soon as their partial pressure falls.

Four duties show the range. Oxygen generation from air uses a 13X type sieve to hold nitrogen and release it on depressurising. Hydrogen purification units use 5A molecular sieve to hold carbon monoxide, methane and nitrogen. Ethanol dehydration runs 3A beds in pressure and vacuum swing, taking ethanol past the point where distillation stops. Heatless compressed air dryers clear water the same way, at the cost of some purge air. For deep drying of natural gas and other process streams, thermal swing remains the normal choice.

Questions on Regeneration Temperature

Can the regeneration temperature be lowered to save energy?

Sometimes, within limits. A lower temperature leaves more water on the sieve, so the bed needs a longer heating time, a drier purge or more sieve to give the same dew point. Where only a moderate dew point is needed, desiccants that regenerate cooler may fit better, as compared in molecular sieve vs activated alumina and molecular sieve vs silica gel.

Why must a molecular sieve bed be cooled before it goes back on line?

A hot bed holds far less water than a cold one. The first gas through it would leave wetter than specified until the bed had cooled itself, and the drying front would already sit part way down the bed. In LNG liquefaction plants, even a short wet pulse can leave ice in the cold box.

What is the hold step in molecular sieve regeneration?

The hold is the time the purge inlet stays at its final temperature after the outlet has caught up. It lets the coolest parts of the bed reach full temperature. Some duties add a second hold part way up the ramp, so one compound leaves before the heat that would break it down. Hold times are set in design and confirmed from temperature records.

How can operators tell that regeneration is complete?

The outlet temperature curve is the main guide, but the proof comes in the next adsorption step. A well regenerated bed stays dry for its full design time. Comparing breakthrough times between towers shows whether one is being under heated. A portable hygrometer on the outlet during a test cycle gives the clearest answer, a method also used to time molecular sieve replacement.

Does 3A need a different regeneration temperature than 13X?

Usually it does. 3A mostly holds water and often serves reactive feeds, so it is regenerated a little cooler. 13X often carries sulfur compounds or CO₂ as well as water and is taken hotter so those leave fully. The duty matters more than the grade label, as set out in molecular sieve types and how to choose between them.

Request a Quote for a Thermal Swing Dryer

To review a regeneration cycle, send SorbiTech the grade and bead size in the bed, the duty and the purge gas composition, the inlet temperature and ramp, and the heating, hold and cooling times. A recorded outlet temperature curve from a recent cycle and the latest breakthrough times are the most useful data of all. Values for a specific unit are agreed in the quotation.